Before

Laser Sintered PVDF and Nylon 11 Tensile Bars

Raw Laser Sintered Surface – Sa 312.63 µin Roughness Scan

After

Laser Sintered PVDF and Nylon 11 Tensile Bars

3D surface roughness scan showing Sa 38.54 µin on laser sintered tensile bar after polishing

Objective

Bel Air Finishing was tasked with developing a surface finishing process for laser sintered PVDF and Nylon 11 impellars, with a strict requirement: the final surface roughness needed to be 125 microinches (µin) or better. The customer required a solution that preserved dimensional accuracy while smoothing the surface for post-process evaluation and potential coating applications.

Part Description Laser Sintered PVDF and Nylon 11 Impellar
Industry3D Print Post-Process – Plastic
3D Printing TechnologyLaser Sintered
MaterialPVDF and Nylon 11
Process TypeSmooth & Polish Surface
Equipment TypeIndustrial 3D Print Smoother, Centrifugal Barrel Finisher/Harperizer, Centrifugal Disc Finisher

Solution

Bel Air tested multiple finishing methods to determine which approach could reliably achieve the target surface finish of 125 µin or better across both PVDF and Nylon 11 impellars. Using a combination of 3D print smoothing, centrifugal barrel finishing (harperizing), and centrifugal disc finishing, the team evaluated each method based on surface refinement, material compatibility, and consistency.

The 3D Print Smoother provided an effective first-pass smoothing operation, gently removing surface texture while preserving part geometry. Centrifugal barrel and disc finishing were then used for deeper refinement and additional surface improvement. Each process was tuned to ensure surface roughness stayed below the 125 µin threshold, allowing the customer to confidently move forward with proven finishing methods for production polishing and mechanical testing.

If you are unsure what equipment and media you require to achieve your desired surface finish, then send us your part, and we will evaluate it and provide you with a metrology report.